Engineering reference

Injection moulding temperature chart — melt, mould and drying

Typical processing windows for the thermoplastics that dominate technical moulding. Values are compiled from machine-maker guidance and material-supplier practice — your specific grade’s datasheet always governs, especially for filled, flame-retardant and impact-modified variants.

MaterialMelt temp (°C)Mould temp (°C)Drying (typical)
PP220–29020–60Usually not required (surface moisture only)
HDPE200–28020–60Usually not required
PS / SB160–23020–60SB: 80 °C · ~3 h if streaking
ABS180–26040–8590 °C · ~3 h · to <0.2% moisture
PC280–32080–100120 °C · 2–4 h · dry until streak-free
PA6 / PA66 (nylon)240–29060–110~100 °C · ~4 h · to <0.15% moisture
PBT240–27060–100120 °C · ~4 h · to <0.02% moisture
POM (acetal)190–23060–120120 °C · ~4 h if regrind/moist storage
PET260–29020–140 (grade-dependent)Dry thoroughly — hydrolysis-critical

Compiled from machine-maker processing guidance (ARBURG/Rapra practical literature) and supplier practice. Glass-filled grades typically run at the upper melt range with hotter moulds.

The three rules behind the table

Hygroscopic resins re-wet fast. Nylon, PC, PBT and PET drink moisture from air — dried material left in an open hopper can be wet again within the hour. Dry to spec, keep hopper loadings matched to consumption, and treat moisture streaks as a drying audit, not a machine fault. Semi-crystalline materials want warm moulds. Their crystals need temperature and time to form; a cold mould freezes an unstable structure that finishes shrinking after moulding — in the customer’s warehouse. The window is a window. Running at the bottom of the melt range saves energy and residence-time risk; the top buys flow for thin walls — a choice, not a default.

Companion tools

These temperatures feed the cycle-time estimator directly, and the drying rules explain half the defects in any moulding shop. Choosing the material itself? Start with the materials guide.

Processed with discipline

Kruger Industries runs dried, documented engineering polymers under SCADA-monitored process control — ISO 9001:2015, material certificates with shipments, Bengaluru, India. Send your drawing; an engineer replies within 48 hours on working days.